Gravity Shaking Table: Reading a Lab Test You Can Scale
A shaking table test tells you two things at once: whether the ore responds to gravity at all, and at what size the response disappears. Most programmes read only the first, run one pass, and then specify a full-scale circuit from a concentrate grade that came from a roughing cut.
What the table is actually separating
Gravity separation works on the product of density difference and particle size. Two minerals with a density ratio above about 1.5 separate cleanly down to roughly 75 µm; below that, the film of water on each particle dominates and everything rides the same band. This is why a laboratory shaking table is a good rougher and a poor finisher, and why the fines you feed it decide whether the test means anything.
Before the table, the sample has to be sized. A PSD from a wet sieve shaker tells you which fractions to test separately, and testing 2 mm feed as one lot hides the fact that the −75 µm half is not separating at all.
The four variables that matter
| Variable | Typical range | Effect |
|---|---|---|
| Stroke length | 8–16 mm on a lab deck | Longer stroke for coarser feed; too long and the bed lifts, losing the stratification |
| Frequency | 280–360 rpm, VFD | Controls how often the bed is re-fluidised; too slow and heavy minerals do not migrate down |
| Table slope | 0–4° plus transverse tilt | Steeper moves more material to tailings and cuts recovery; flatter raises grade at lower throughput |
| Wash water | 0.3–1.0 m³/h, just enough to see the bands | Too much dilutes the pulp and drags heavies into tailings |
On a 1100 × 500 mm lab deck the working envelope is narrower than the general ranges above, and smaller than most operators expect: 20–80 kg/h at −2 mm feed, and the throughput moves with liberation long before it moves with the motor.
Change one at a time and keep the feed rate constant. Tables are sensitive to feed rate in a way that surprises people: a 20% swing in solids per hour moves the cut point more than a 2° change in slope.
Reading the bands, not just the weights
Watch the table while it runs. A well-set table shows a narrow, sharply defined heavy band along the concentrate edge, a middlings zone that is visibly transitional, and a tailings sheet that is uniformly light. What you are diagnosing:
| What you see | Likely cause | Adjustment |
|---|---|---|
| Heavy band smeared across half the deck | Too much feed, or slope too flat | Reduce feed, increase slope slightly |
| Clean concentrate but low recovery | Wash water high, or slope too steep | Cut water, flatten slope, re-run |
| Middlings zone missing entirely | Liberation is poor at this size | Re-grind a split, or accept a rougher cut |
| Concentrate contaminated with light gangue | Stroke too long for the size fraction | Shorten stroke, re-clean the concentrate |
Mass pull is the number people forget to record
A concentrate grading 40% Au-bearing mineral means nothing without the mass that produced it. Record concentrate mass, middlings mass and tailings mass, and calculate recovery from assays of each — not from the feed alone. A single-pass table test typically pulls 5–30% of the feed mass as concentrate plus middlings; if your number is outside that, the table is either mis-set or the ore has no gravity response.
Plot grade against recovery for each of three or four cuts. The shape of that curve, not any single point, is what a flowsheet is designed from — the same logic that applies to recovery in any unit operation.
One pass is not a flowsheet
A table rougher followed by a cleaner on the concentrate is the minimum configuration that produces a saleable or downstream-ready product. Testing only the rougher gives an optimistic recovery at an unusable grade; testing only a cleaner gives a good grade at a recovery the plant will never see. Run the rougher, then re-run its concentrate, and report both stages with their mass balances.
When the table is the wrong tool
- Below 50 µm with a small density difference. Centrifugal units generate the force the table cannot; a table will report the value mineral as tailings.
- Strongly paramagnetic minerals. A wet high-intensity magnetic separator is the direct test, and the two are often compared before a flowsheet is fixed.
- Sulphide flotation feeds. If the value reports to a floatable sulphide, a batch flotation cell answers the metallurgical question faster and at a finer size.
Tables also scale non-linearly. Deck area per tonne of feed increases as the feed gets finer and as the density difference shrinks, so a test that works at 50 kg/h does not automatically multiply to 5 t/h on the same deck configuration. Design from the unit-area figure measured in the test, and treat the pilot unit as a data source rather than a scale model — the reasoning behind any process flowsheet built on test work.
Send the size analysis, the mineralogy and the target concentrate grade, and we will propose the rougher–cleaner test sequence and the deck settings to start from.