Ring and Puck Pulverizer: How Fine Does an Assay Sample Need to Be?

An assay is only as good as the 100 g that reaches the laboratory, and that 100 g is only as good as the pulverising step. A ring and puck pulverizer will happily produce a fine powder in ninety seconds that is completely unrepresentative — because the bowl was too small for the sample, the grinding media contaminated it, or the sulphides oxidised while it got hot.

Why 75 µm became the number

Below roughly 75 µm (200 mesh), most rock-forming minerals are liberated enough that a 30 g assay aliquot behaves like the whole sample. That is the practical reason the convention stuck, not any law of nature. For coarse gold it is nowhere near enough, and for a quick head grade on a homogeneous ore you can get away with coarser.

The number to work with is not “how fine” but “how fine, for this sample mass”. A 75 µm product from 1 kg and from 50 g are not equivalent when gold is present at gram-per-tonne levels.

Sample mass sets the bowl, not the other way round

Sample mass Typical bowl Practical grind Notes
20–50 g 100 mL 1–2 min Fine for homogeneous base-metal ores
100–200 g 250 mL 2–4 min Standard head assay, duplicates retained
500 g–1 kg Larger bowl or split first In stages Overloading stalls the puck and grinds unevenly
Coarse gold 1 kg+ or screen metallics Coarse crush only Pulverising 100 g of a gold ore is how nugget effect becomes a bad resource estimate

Overloading is the most common mistake. A puck that cannot move freely does not grind the whole charge; it grinds the part it can reach and leaves a coarse heel in the corner that gets scooped last into the assay packet.

The working point on a bench-top vibratory unit is a 250 mL bowl with a 50–250 g charge and a feed already below 6 mm. One to five minutes of grinding gets most ores to 75–90 µm; 45 µm is reachable with an extended run, at the cost of more heat and more wear — which is the trade-off the next section is about.

Contamination you can measure

Grinding media wear into the sample, and the direction of the bias is predictable:

  • Chrome steel: cheapest and toughest, adds Fe and Cr. Fine for base metals at percent levels, unacceptable for chrome ore or a Fe-sensitive suite.
  • Tungsten carbide: the workhorse for hard rock. Adds W and Co — which matters if tungsten or cobalt is the element of interest, an easy trap in battery-recycling and W-ore work.
  • Agate or ceramic: low contamination but slow and brittle. Reserved for trace and PGM work.

Whichever you use, report it. When two laboratories disagree by 15% on the same sample, the grinding media is one of the first three things to compare.

Heat is a chemical change

Grinding energy goes into the sample as heat. Two or three minutes of vigorous pulverising in a sealed bowl is enough to warm a sulphide concentrate past the point where sulphur starts to oxidise and mercury starts to leave. If your suite includes S, Hg, As or any volatile, grind in short bursts with a pause, or use a mill with cooling. A head grade that drifts downward between the coarse reject and the pulp is a grinding problem, not an analytical one.

Check the fineness instead of assuming it

Take 20 g of the pulp and wash it through a 75 µm sieve. What stays on the screen is your oversize, and it should be under a few percent. If it is 15%, the pulp is not ready and the assay will under-report grade because the coarse fraction is under-digested in the acid attack. A wet sieve shaker makes this a five-minute check rather than a hand-washing exercise.

The sequence that avoids most of this

  1. Crush to 2 mm in a jaw crusher — the pulveriser is not a crusher and will not forgive a 10 mm feed.
  2. Riffle split to the mass you actually need, retain the reject.
  3. Pulverise in short bursts, sized bowl, media chosen against the element list.
  4. Verify oversize on a 75 µm screen.
  5. Record bowl, media, time and oversize in the report.

If the same pulp is going into a leach rather than an assay, stop at the crush stage — see the bottle roll test unit. Pulverising to 75 µm before a leach changes the kinetics so much that the result cannot be scaled to a plant grinding to 150 µm. The pulp density you set in the bottle, and the recovery calculation that follows, both assume the feed size is the one the flowsheet will produce.

Send the element list, the expected grade range and the sample mass, and we will specify bowl size, media and grind time for the suite you are running.