Laboratory Jaw Crusher: Setting the Crush Before a Test Means Anything

Most disappointing leach tests trace back to the crusher, not the chemistry. If the sample reaching the bottle is 6 mm top size while the flowsheet assumes 2 mm, the leach runs slow, the recovery curve flattens, and the result gets filed as a metallurgical problem when it is a comminution one. The laboratory jaw crusher is the first place a test programme is either representative or wrong.

Three jobs, one machine

Crushing has to deliver three separate things, and they pull in different directions:

  • Liberation. Grain boundaries have to open enough for the lixiviant to reach the value mineral. Too coarse and the leach is diffusion-limited; the recovery curve keeps climbing for days and never plateaus.
  • Homogeneity. The 200 g you send for assay must represent the 20 kg in the drum. That is a sampling problem, and crushing to a finer top size is what makes splitting honest.
  • Absence of damage. Over-crushing creates fines that report differently in the next unit operation, generates dust you cannot weigh back, and adds iron or manganese from the plates themselves.

Setting the closed side

Work backwards from the test, not forwards from the machine. The table below is where most programmes should start; adjust once you have a size analysis.

Test Target feed Starting CSS What goes wrong
Bottle roll or agitated leach 100% passing 2 mm 2–3 mm Oversize survives the whole test and under-reports recovery
Head assay / multi-element 2 mm, then pulverise to 75 µm 2–3 mm Pulveriser overloaded, incomplete grind, biased assay
Gravity or table test 1–2 mm 2 mm Fines blind the table and inflate the concentrate mass
Flotation (after grinding) 2–3 mm to the mill 3 mm Grinding time set by feel instead of by P80
Agglomeration / column test −12.5 mm 12–15 mm Too fine a feed agglomerates into marbles and floods

Set the gap with the machine running empty, then check it by sieving a 1 kg portion — not by reading the scale on the adjuster. Jaw plates wear, and a gap that measured 2 mm when new can sit at 3.5 mm after a few tonnes of quartz.

The hardware sets the practical window. A bench-top single-toggle unit with a 100 × 60 mm feed opening and a 1–10 mm handwheel adjustment takes 40 mm lump or drill core in one pass and lands at 2 mm in two — which is why the crush stage is rarely the bottleneck and the split stage usually is. Mn13 plates are reversible, so rotate them before they are worn through, not after.

Over-crushing is not free

Every extra pass adds fines you did not intend. In a leach that matters twice: fines leach faster, so the test looks better than the plant will, and they are harder to filter, so the solid–liquid step downstream behaves worse than the flowsheet predicts. In an assay it matters once but badly: dust lost to the collector is usually the finest, highest-grade fraction, and losing it biases the head grade low.

Crush in stages instead. A single pass from 50 mm to 2 mm produces a wider size distribution and more fines than 50 → 10 → 2 mm, and it is harder on the plates.

Plate material is part of the result

Manganese steel plates are the default because they are tough, and they shed iron and manganese as they wear. For base-metal work at percent levels that is noise. For gold, platinum group metals or any trace-element suite, it is contamination that shows up as a suspiciously high Fe value and a low-grade tail you cannot explain. Use ceramic or tungsten carbide jaws for trace work, and state the plate material in the test report — reviewers ask.

Split before you pulverise

Crushing to 2 mm makes a riffle split defensible; quartering a 20 kg heap with a shovel does not. Split to 1–2 kg for pulverising, retain the reject, and keep the reject labelled with its mass. When the assay comes back anomalous, the first question is always whether the split was representative, and the only way to answer it is to have the material left.

Checklist before the sample leaves the crusher

  • Gap measured cold, then verified by sieving a portion.
  • Whole sample passed, not just the easy part — no oversize returned to the stockpile.
  • Machine cleaned between samples; a brush and compressed air, not a quick shake.
  • Split mass and reject mass recorded.
  • Top size recorded as a measured P100, not as the nominal gap.

From here the sample goes to the ring and puck pulverizer for assay, or straight into a bottle roll leach if the work is metallurgical. If the programme covers gravity or magnetic separation as well, a wet sieve shaker closes the loop by giving you a size analysis you can trust.

Send the sample type, the test you intend to run and the top size you need, and we will confirm the jaw setting and the plate material before the first pass.